TheBulkLab

Newsletter and Process Notes

Production technology, read for process.

A weekly watch on production technology across batteries, semiconductors, ceramics, catalysts, MOFs, chemicals and advanced materials — plus monthly Process Notes that read research and patents for process.

Finding the Right Dispersant Dosage for a Ceramic Slurry

Free sample. This Process Note is open to everyone. New monthly Process Notes are available individually for US$4.99, no account needed. Join the Free Weekly Newsletter to hear when each one is published.

Dispersant dosage is one of the cheapest variables in a ceramic slurry and one of the most often set by habit: a percentage inherited from an earlier product, a supplier datasheet, or “what worked last time”. When a tape-casting or slip-casting slurry starts to drift — higher viscosity, settling, cracked or warped sheets — the dispersant is a sensible first suspect. This guide sets out how to find a working dosage, what the curve should look like, and which side effects to watch for.

What the dispersant is actually doing

Fine ceramic particles attract each other and form agglomerates and networks. A dispersant adsorbs on the particle surface and keeps neighbours apart, electrostatically, sterically, or both. Too little leaves bare surface and a strongly structured, high-viscosity slurry; enough gives the lowest viscosity the formulation can reach; too much leaves free polymer or salt in the liquid, which can raise viscosity again or change the chemistry of the slurry. Tape-casting quality depends heavily on slurry rheology and on how the slurry flows under the blade, as the 2016 review by Jabbaribehnam and co-workers emphasises — so the dispersant sits upstream of almost every sheet property.

The optimum is a property of the system, not of the dispersant

Published work shows how much the right dosage varies. Sever and co-workers (Transactions of FAMENA, 2018) compared three dispersants in 70 wt% alumina suspensions over 0.1–1.25 wt% and found very different optima: about 0.75 wt% for an ammonium polymethacrylate, 0.3 wt% for citric acid and only 0.1 wt% for Tiron. Zhang, Su and Button (Journal of the European Ceramic Society, 2004) reached 84 wt% solids in an aqueous alumina suspension with an ammonium polyacrylate at an optimum of just 0.14 wt%, giving about 0.30 Pa·s at 100 1/s — and reported that adding more dispersant increased viscosity.

Particle size matters as much as chemistry. A coarse-grained simulation study of barium titanate slurries with a phosphate-ester dispersant (Nakata and co-workers, arXiv, 2021) found very high low-shear viscosity at the lowest dispersant level, near-Newtonian behaviour at higher levels, and an appropriate amount between them; the authors also point out that smaller particles, with more surface area, need more dispersant. A dosage that worked for one powder lot or grade can therefore be wrong for the next, even with the same supplier and the same nominal material.

Finding a working dosage: a practical sequence

  1. Fix everything else. Use one powder lot, one solids loading, one mixing or milling procedure and one temperature. Add binder and plasticiser after this step, not before — they change the rheology and can hide the dispersant effect.
  2. Run a dosage series. Five or six levels spanning the supplier range, expressed on powder weight (or better, per unit of powder surface area if you know the specific surface area).
  3. Measure a full flow curve for each level, with the same pre-shear and rest step. Plot viscosity at a low and a high shear rate against dosage. The optimum is usually a minimum or a flat floor; the low-shear value responds most strongly.
  4. Check stability, not just viscosity. Repeat the measurement after a realistic hold time and look for settling. A slurry at minimum viscosity that settles overnight is not a working slurry.
  5. Choose slightly above the minimum. In production, powder surface area varies. Sitting just on the rising side of the minimum is often more robust than sitting at its exact point — but confirm on your own data, because excess dispersant has its own costs (below).
  6. Repeat when the powder changes. A new grade, supplier or milling time is a new system.

Side effects that a viscosity curve will not show

Dispersant choices reach beyond rheology. In aqueous tape casting of barium titanate, Isaka, Shiomi and Inaoka (Journal of the Society of Materials Science, Japan) found that adding dispersant lowered the slurry pH and increased Ba²⁺ leaching. Higher binder content increased shrinkage and warpage of the fired sheets, the dispersant effect on warpage was strongest at high binder content, and the authors linked warpage to differences in particle packing between the top and bottom of the sheet. In other words, a dispersant level that looks fine in the rheometer can still show up later as a chemistry or packing problem in the fired part.

Typical things worth checking alongside viscosity:

  • pH drift after dispersant addition, and any ion leaching from reactive powders.
  • Foaming and wetting behaviour on the carrier film or mould.
  • Green density and its uniformity through the thickness.
  • Burnout residue, especially in thin sheets and multilayer parts.
  • Interaction with the binder: some binder systems flocculate a well-dispersed slurry, others stabilise it further.

When the slurry drifts in production

If viscosity or casting quality changes with no recipe change, compare the flow curves of a good and a bad batch measured under the same protocol. A difference mainly at low shear points to dispersion state — powder surface area, dispersant dosage, mixing energy or water quality. A difference across the whole curve points more often to solids loading or binder. Comparing measured curves with what the formulation should give is the basis of our Quick Check and Process Review services.

Practical takeaways

  • Find the optimum dosage experimentally for each powder grade; published optima vary several-fold between dispersants and systems.
  • Judge by the full flow curve and by stability over time, not by one viscosity reading.
  • Expect excess dispersant to cost you — in viscosity, chemistry or downstream defects.
  • Re-check dosage whenever powder lot, grade or milling changes.

Sources

  • I. Sever, I. Žmak, L. Ćurković, Z. Švagelj, “Stabilization of Highly Concentrated Alumina Suspensions by Different Dispersants”, Transactions of FAMENA 42(3), 61–70, 2018. doi.org/10.21278/TOF.42304
  • D. Zhang, B. Su, T. Button, “Preparation of concentrated aqueous alumina suspensions for soft-molding microfabrication”, Journal of the European Ceramic Society 24, 231–237, 2004. doi.org/10.1016/S0955-2219(03)00241-3
  • H. Nakata, T. Kiguchi, O. Hino, “Investigation of the effect of surface phosphate ester dispersant on viscosity by coarse-grain modeling of BaTiO3 slurry”, arXiv:2111.08876, 2021. arxiv.org/abs/2111.08876
  • Y. Isaka, H. Shiomi, K. Inaoka, “Effects of the Amount of Dispersant and Binder on Slurry and Sheet Properties in Aqueous Tape Casting of Barium Titanate”, Journal of the Society of Materials Science, Japan, 60(6), 500–503. jsms.jp
  • M. Jabbaribehnam, R. Bulatova, A. I. Y. Tok, C. Bahl, E. Mitsoulis, J. H. Hattel, “Ceramic tape casting: A review of current methods and trends with emphasis on rheological behaviour and flow analysis”, Materials Science and Engineering B 212, 39–61, 2016. doi.org/10.1016/j.mseb.2016.07.011

This article is general technical commentary, not advice for a specific process. Validate any change under your own operating conditions.