Sample Quick Check memo
A shortened Quick Check memo built on a fictional ceramic tape-casting case — the format, depth and tone you receive for one formulation and one clear question.
After switching to a new lot of the same alumina grade, an aqueous tape-casting slurry became noticeably thicker in the mixer and the cast tape showed edge cracking. The recipe was unchanged. Is the new lot the cause, and what should be checked before adjusting the recipe?
| What the data shows | What it does not show |
|---|---|
| Lot B is about 2.4× more viscous than lot A at 1 1/s, but only about 1.2× at 100 1/s and 1.1× at 1000 1/s. | Whether the difference comes from the powder itself or from how it was dispersed — the flow curve alone cannot separate the two. |
| The certificates give a specific surface area of 7.8 m²/g for lot A and 9.6 m²/g for lot B (fictional values). | Particle-size distribution or surface chemistry beyond the certificate values. |
| Dispersant was dosed at 0.5 wt% on powder for both lots, so dispersant per unit of powder surface fell by about 19% with lot B. | The adsorption limit of this dispersant on this powder; no dosage series is available yet. |
| # | Cause | Why it fits | Confidence |
|---|---|---|---|
| 1 | Dispersant under-dosed for the higher surface area of lot B | Excess is concentrated at low shear; surface area rose about 23% while dosage stayed fixed | Moderate |
| 2 | Different surface chemistry or soluble ions in lot B | Would also change dispersion; not ruled out without pH and conductivity data | Low |
| 3 | Measurement difference between the two runs | Same protocol reported; worth confirming before acting | Low |
One round of written follow-up questions is included. The background to step 1 is explained in our Process Note Finding the right dispersant dosage for a ceramic slurry.
By request
Quick Checks are taken on by request, as time allows. Describe your question briefly and you will hear back about fit, timing and price.